Abstract

Wildcard week: nanofabrication.

This week, as a wildcard, I decided to bring my own expertise in nanofabrication to the table. In an ideal world, I think a class on “How to Make Almost Anything” would include at least an introduction to nanofabrication. On the other hand, I completely understand that access to clean room facilities is generally restricted, requires lenghty training, and is expensive. Furthermore, it is not really necessary: such a plethora of integrated circuits are so easily available, for so cheap, that there isn’t really much point in fabricating your own (and also, the expertise to do so properly is not at all easy to acquire). The only situation that justifies use of clean room facilities is trying to implement completely new computing paradigms that simply cannot work on existing IC architecture.

For those interested to go beyond my introduction here, I highly recommend this Veritasium video that explains well the basics of the field, as well as the most advanced developments in the field using ASML EUV machines. Such machines are so complicated and expensive that they really only make sense in an industrial environment, so none is available at MIT (in fact, only a few dozen have ever been made and deployed to production). The nanofabrication I am presenting this week makes use of much more conventional (and less powerful) methods.

While expensive to start with, nanofabrication scales really well in terms of cost: fabricating many integrated circuits on 6 or 8 inch wafer takes (almost) the same amount of materials and labour as a 1 inch piece - hence, the cost per device is much lower when nanofabrication is done at a large scale rather than at low scale.

The clean room

First, a little bit about the place where this is all done: the clean room. As the name says, nanofabrication means fabricating structures at the nano (10−910^{-9} meters) scale - for the devices to work well, they need to be perfect down to this scale. For comparison, a human hair has a diameter of 50 to 100 microns (so 100,000 times larger), and single spec of dust is also in the range of microns (so about 1000 larger). Your usual room is full of such dust particles, so they would stick very easily to your device - and any such particle is capable of ruining your device completely. You need to get rid of those completely Well, almost. .

This is why the clean room is necessary: to get rid of all these unwanted particles in the atmosphere. Believe it or not, we are one of the worst sources of dust out there (due to having skin and hair), so any bit of our bodies needs to be completely covered. Hence, we wear this head-to-toe bunny suit, made of a special material that doesn’t emit or let such particles through This is why access is restricted to the clean room: people need to know how to properly dress before even entering the door. . Then, you need a proper ventilation system that can quickly remove any particles still left and not bring them onto your devices Very complex as well: the one at MIT.Nano takes up the entirety of floors 2 and 4 of the building .

We are very fortunate to have MIT.Nano available to us: a very modern and very well organized clean room with most of the nanofabrication equipment you could ever need for research. Access is available to all MIT community, but strictly regulated and charged according to use. This is a class 100 clean room: this means that in a cubic foot of air there are no more than 100 particles larger than half a micron While it’s difficult to grasp the number without a comparison, trust me, it is extremely clean .

Bunnysuit
Me gowned up in a bunny suit. Also notice the metallic benches (so as not to emit particles) with holes all around (to allow particles to pass through to the ground rather than accumulate on the bench).

The three basic nanofabrication processes

These are the three things you can do in the clean room, boiled down to the basics:

  • Create a pattern;
  • Add some material (deposition);
  • Remove some material (etching).

All of these are done on top of a substrate, which is usually a solid, several hundred micron thick piece of material. Most nanofabrication is done on sillicon substrates (used for its semiconducting properties), though depending on the application one can use other substrates (glass, quartz, sapphire, etc).

All of these proceses come in various flavors and methods that I will not delve further into. For this week I will focus my attention on the first two, as my favorite etching method is unfortunately unavailable at the moment :(

My goal for this week

I want to start from a sillicon chip and deposit a nanometer-thick metallic pattern in the shape of a butterfly. The butterfly picture I am starting from is shown below.

Butterfly
PNG of a butterfly that I nanofabricated on a Si chip this week.

Depositing the metal

While this is one of the last steps in the fabrication process, I prefer describing the deposition first, as it will shed some light onto why the previous steps are done the way they are. I deposit the metal using an ultra-high vacuum sputtering system. This works as follows:

  • The substrate is placed in an ultra-high vacuum chamber (10−910^{-9} Torr) Atmospheric pressure is 760 Torr. .
  • The chamber is flushed with ultra-high purity Argon gas.
  • A high voltage (up to 500 V) is applied in order to strike a plasma in the Argon.
  • The argon atoms hit, at a very high speed, a “target” made of the desired deposition metal, and eject atoms out of that target.
  • The ejected metallic atoms are accelerated towards the substrate using electric and magnetic fields. When they hit the substrate, they stick to it.

The ultra high vacuum ensures that the deposited film is uniform in thickness down to the nanometer scale. The use of high voltages for ejecting and directing atoms makes this a violent process: this is good since it gives rise to very strong bonds to the substrate and very high quality films. This is also bad since it has a lot of randomness. In particular, it is not directional at all: relative to the substrate, atoms come in at all angles and from all directions. There is no way to ensure any sort of directionality. The metal will be deposited everywhere on the substrate. This is why a patterning step is necessary besides the metal deposition.

Digital design for patterning

At the digital level, patterning a silicon chip/wafer is very similar to PCB design - one needs to specify the traces where material is wanted and where it is not wanted. In fact, Gerber is one of the valid file format inputs, though most people prefer DXF and GDS files. A particular advantage for GDS is the existence of well-maintained Python libraries for GDS pattern generation.

In some sense, nanopatterning design is more flexible than PCB design: you can have as many layers as you want, and are not constrained to a few or to powers of two - yet, every new layer will mean an additional round of deposition, patterning, and/or etching. On the other hand, it is less streamlined, as there are no predefined footprints to make use of. Furthermore, there are no prepackaged components to assemble/solder onto this pattern: every “device” you make is some geometric arrangement in 3D, at the nanoscale, of some materials (not to mention that there is no notion of soldering at those scales!).

I put the powers of these Python libraries to test by converting the picture of the butterfly into a GDS pattern. This Python script Generated inside MIT Parley using Claude 5.5 Opus. takes a black-and-white PNG file and converts it to a pattern of a specified pixel size (in this case, 2 microns; could have gone down to 0.5 microns, as explained below) and of a specified total size (in this case, 15 mm - it just needs to be lower than the substrate size, 25 mm). The output GDS file used for patterning is attached here and a screenshot of some details is shown below.

Butterfly overview Butterfly detail
Overview and detail of the generated photolithography pattern, shown with a scale bar.

Photolithography

Now that we have a pattern, how do we actually turn it into something physical? How do we make sure that in the end, metal is deposited only in the areas specified by the pattern and not elsewhere? Unfortunately there is no micron thick endmill that can dig in by a few nanometers! The key is that, prior to metal deposition, we need to define a “mask”: some other material, that we would be able to specify in this pattern, that would exist everywhere on our substrate except where we want the metal to be deposited. This mask should also be easy to remove once our metal is deposited.

Such masks are made out of what is called “photoresist”. Photoresists are polymers that can coat the substrate (through a process called spin-coating). They are sensitive to blue light, meaning exposure to blue light causes a reaction that locally changes their chemical properties (this is why photolithography is done in rooms with orange light and no windows). In particular, only the exposed photoresist becomes soluble in another substance, called the developer. The typical patterning workflow is the following:

  • Spin-coat the photoresist onto the substrate;
  • Expose to blue light according to the pattern;
  • Remove the exposed photoresist using the developer;
  • Deposit metal onto the pattern (according to the above);
  • Dissolve remaining photoresist using an organic solvent (and remove metal in unwanted regions - this is called lift off).

This workflow is illustrated in the figure below.

Photolithography
Process diagram for metal patterning with photolithography via liftoff.

Exact recipe

For the sake of exactness, below is the full process flow used for fabricating the butterfly:

  • Clean the substrate with acetone and IPA; bake for a few minutes at 110 C to remove moisture.
  • Spin coat the AZ nlof 2020 photoresist at 4000 rpm for 1 minute, followed by a soft bake of 75 s at 110 C.
  • Expose the pattern on a Heidelberg MLA 150 machine, using the inverted pattern, with the 375 nm laser, with a dose of 340 mJ/cm^2 and a defocus of -3. Follow with a post-exposure bake of 75 s at 110 C.
  • Develop the pattern with the AZ 300 MIF developer, for 90 s, followed by a 3 beaker water rinse.
  • Clean the sample prior to deposition with an oxygen plasma at 100 W, 2 sccm, for 1 minute.
  • Deposit 5 nm of Ta, followed by 10 nm of Pt, by sputtering.
  • Lift off the metal and remove the photoresist by sonication in acetone for 10 minutes, then in IPA for 1 minute.

The result

Below is a picture of my chip in real size, as well as microscope images of it, showing the level of precision and the sharpness of this pattern. There are occasional specs of dust here and there but I would call this a successful patterning!

Butterfly chip Butterfly overview Butterfly detail 1 Butterfly detail 2
Images of the butterfly chip under various levels of magnification.